24小时热门版块排行榜    

查看: 1107  |  回复: 4

lxzlhh

银虫 (初入文坛)

[求助] ANSYS计算焊接应力场,熔池部分热应力非常小,请高手解答 已有2人参与

用ANSYS计算焊接应力场,熔池部分热应力非常小,网上说这是由于这部分是液体(零应力状态),这个我可以理解,但是我想知道ANSYS是怎么判断它是熔池的,我在输入参数时并没有输入熔点、液相线等参数,我也改变过弹性模量、热膨胀系数等参数,但是熔池部分热应力一直很小(接近零),求高手帮我解答,小弟感激不尽!!!!
温度场计算参数:
MPTEMP,1,20,250,500,750,1000,1500,1700,2500
MPDATA,DENS,1,1,7820,7700,7610,7550,7490,7350,7300,7090
MPDATA,C,1,1,460,480,530,675,670,660,780,820
MPDATA,KXX,1,1,50,47,40,27,30,35,140,142
力学参数:
mptemp,1,20,250,500,750,1000,1500,1700,2500
mpdata,prxy,1,1,0.28,0.29,0.31,0.35,0.4,0.45,0.48,0.5
mpdata,alpx,1,1,1.10e-05,1.22e-05,1.39e-05,1.48e-05,1.34e-05,1.33e-05,1.32e-05,1.31e-05,1.32e-05,1.31e-05
mpdata,ex,1,1,2.05e+11,1.87e+11,1.50e+11,7.00e+10,2.00e+10,1.90e+10,1.80e+10,1.20e+10

MP,REFT,1,20
MP,REFT,2,20

TB,BISO,1,6,2,

TBTEMP,20
TBDATA,,2.20E+08,2.05E+10,,,,
TBTEMP,500
TBDATA,,1.30E+08,1.50E+10,,,,
TBTEMP,750
TBDATA,,4.00E+07,7.00E+09,,,,
TBTEMP,1000
TBDATA,,2.50E+07,2.00E+09,,,,
TBTEMP,1700
TBDATA,,1.00E+06,1.80E+09,,,,
TBTEMP,2500
TBDATA,,1.00E+05,1.20E+09,,,,

ANSYS计算焊接应力场,熔池部分热应力非常小,请高手解答
ansyss.JPG
回复此楼

» 猜你喜欢

» 本主题相关价值贴推荐,对您同样有帮助:

已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

lxzlhh

银虫 (初入文坛)

图片没传好,补上
ANSYS计算焊接应力场,熔池部分热应力非常小,请高手解答-1
图片1.png

2楼2015-02-09 20:32:11
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

wb1895

木虫 (正式写手)

【答案】应助回帖

判断,关键看你屈服强度随着温度的变化,屈服了应力就很小。你修改其他参数没什么影响的。
你去掉屈服强度这个参数看看,就知道了。
3楼2015-02-13 21:06:13
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

yangzizhang

新虫 (初入文坛)

【答案】应助回帖

我觉得输入热参数计算温度场时应该再加上换热系数或者是热焓,计算时通过观察温度场的形态来判断熔池,焊接过程中的熔池并不是通过应力分布来判断的,而是温度,超过了钢材的熔化温度,那自然就是熔池部分了,你最好把温度场的图也发上来,这样才好判断啊
4楼2015-03-08 13:54:02
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

xinghuocumt

新虫 (小有名气)

请问楼主解决,液态熔池零应力的设置问题了吗
5楼2018-07-19 22:07:47
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖
相关版块跳转 我要订阅楼主 lxzlhh 的主题更新
信息提示
请填处理意见