[交流] 【求助】纳米纤维的BET结果分析

t-method 计算没有微孔, 而DR,HK, SF都计算出微孔,应该用哪个?在小木虫看到t-method, DR,HK, SF都是分析微孔的方法,他们有什么区别和特别的应用吗?

BJH Method Cumulative Adsorption Pore Volume 怎么会比总的孔容 Total Pore Volume for pores 还大?

以前没做过这方面分析,请专家帮忙分析一下?

                               SURFACE AREA DATA

Multipoint BET..............................................  9.974E+01  m²/g
Single Point BET............................................  8.701E+01  m²/g
Langmuir Surface Area.......................................  1.817E+02  m²/g
BJH Method Cumulative Adsorption Surface Area...............  1.991E+02  m²/g
BJH Method Cumulative Desorption Surface Area...............  8.357E+01  m²/g
DH Method Cumulative Adsorption Surface Area................  2.079E+02  m²/g
DH Method Cumulative Desorption Surface Area................  8.732E+01  m²/g
t-Method External Surface Area..............................  9.974E+01  m²/g
t-Method Micro Pore Surface Area............................  0.000E+00  m²/g
DR Method Micro Pore Area...................................  1.523E+02  m²/g

                                PORE VOLUME DATA

Total Pore Volume for pores with Diameter
less than 7881.2 Å at P/Po = 0.99757........................  1.072E-01  cc/g
BJH Method Cumulative Adsorption Pore Volume................  1.450E-01  cc/g
BJH Method Cumulative Desorption Pore Volume................  7.384E-02  cc/g
DH Method Cumulative Adsorption Pore Volume.................  1.439E-01  cc/g
DH Method Cumulative Desorption Pore Volume.................  7.338E-02  cc/g
t-Method Micro Pore Volume..................................  0.000E+00  cc/g
DR Method Micro Pore Volume.................................  5.412E-02  cc/g
HK Method Cumulative Pore Volume............................  3.255E-02  cc/g
SF Method Cumulative Pore Volume............................  3.395E-02  cc/g

                                 PORE SIZE DATA

Average Pore Diameter.......................................  4.300E+01  Å
BJH Method Adsorption Pore Diameter (Mode)..................  1.380E+01  Å
BJH Method Desorption Pore Diameter (Mode)..................  1.946E+01  Å
DH  Method Adsorption Pore Diameter (Mode)..................  1.380E+01  Å
DH  Method Desorption Pore Diameter (Mode)..................  1.946E+01  Å
DR  Method Micro Pore Width   ..............................  1.813E+02  Å
DA  Method Pore Diameter (Mode).............................  1.880E+01  Å
HK  Method Pore Width    (Mode).............................  1.362E+01  Å
SF  Method Pore Diameter (Mode).............................  2.547E+01  Å

本帖关键词:Adsorption Pore BET Volume Method
回复此楼

» 猜你喜欢

» 本主题相关商家推荐: (我也要在这里推广)

已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

xiaonade

木虫 (小有名气)

至于你说的Total Pore Volume for pores ,别忘了下面还有一行“with Diameter less than at P/Po = 0.99757.”也就是说他所测得的孔容只是半径小于7881.2 Å 的孔的总孔容。并不是全部孔的孔容,当然会小了。
   只是个人看法,我也是个初学者,如果有不对的地方还请指正啊~~~
3楼2009-12-03 16:05:42
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖
查看全部 5 个回答

xiaonade

木虫 (小有名气)

★ ★ ★
小木虫(金币+0.5):给个红包,谢谢回帖交流
骑着蜗牛追火箭(金币+2,VIP+0):谢谢 12-3 17:12
1、固体材料比表面积大于1 m2/g ( BET;Langmuir)。
     
  2、微孔分布:0.45 — 1.7 nm;
     
  微孔孔容:0.0001 cm3/g(Horvath-Kawazoe、MP-Method)。
     
  3、中孔分布:1.7 — 300 nm;
     
  中孔孔容:0.0001 cm3/g (BJH-Method、t-Plot Method、DET Theory)。
以Kelvin方程为基础的方法(如BJH法)是与孔内毛细管凝聚现象相关的,所以
它们可应用于介孔分布分析,但不适用于微孔填充的描述,甚至对于较窄的介孔
也不正确。
• 其它的经典理论,即如杜平宁-兰德科维奇(DR)法,和半径验处理的方法(如
HK和SF法)仅致力于描述微孔填充而不能应用于中孔分析.

这样看来,你测得这个绝对可以排除T-method的影响了。
2楼2009-12-03 16:01:53
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

tjpu302

木虫 (正式写手)

Niu_HT

谢谢xiaonade的解答

我还有个问题不清楚,如果想说明微孔比表面积多大该用t-Method还是DR method的值?
4楼2009-12-03 16:52:19
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

fdgudong

铁杆木虫 (正式写手)

★ ★
小木虫(金币+0.5):给个红包,谢谢回帖交流
骑着蜗牛追火箭(金币+1,VIP+0):谢谢 12-3 17:12
t方法用来计算微孔孔容,根据材料性质不同,取点范围也不一样。用BET方法计算比表面积首先要看C常数和Y轴截距是不是为正,其次还要线性>0.9999