24小时热门版块排行榜    

查看: 660  |  回复: 4
当前主题已经存档。
当前只显示满足指定条件的回帖,点击这里查看本话题的所有回帖

yihanfan

金虫 (小有名气)

[交流] ZSM-5如何制备HZSM-5

ZSM-5如何制备HZSM-5?
想请教一下,是否将ZSM-5浸渍于铵离子溶液中可以将其转变为HZSM-5.
回复此楼
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

yihanfan

金虫 (小有名气)

非常感谢

非常感谢你的建议,不知道是否能够再详细点,或者有篇专门文献。
3楼2008-05-25 22:18:42
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖
查看全部 5 个回答

zds1301

铁杆木虫 (著名写手)

★ ★
^_^@^_^(金币+2,VIP+0):非常感谢
5wt% NH4Cl 或NH4NO3;
1:10=ZSM-5:NH4Cl (体积比);
过量浸渍3次;
过滤,洗涤至不含Cl离子为止,干燥,即可!
2楼2008-05-25 22:12:13
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

zds1301

铁杆木虫 (著名写手)


^_^@^_^(金币+1,VIP+0):多谢!
给你个文献,
Applied Catalysis A: General 185 (1999) 41–52
ZSM-5 zeolite with enhanced acidic properties
R. Le Van Mao , T.S. Le, M. Fairbairn, A. Muntasar, S. Xiao, G. Denes
Concordia University, Department of Chemistry and Biochemistry and Laboratories for Inorganic Materials,
1455 De Maisonneuve West, Montreal, Que. H3G 1M8, Canada
Received 27 January 1999; accepted 31 March 1999
Abstract
ZSM-5 zeolite, when doped with fluorine species in relatively low concentration using ammonium fluoride as precursor,
and subsequently activated stepwise at high temperature, shows an enhanced surface acidity because of: (i) the formation of
new Bronsted acid sites; and (ii) the strengthening of some acid sites of the parent zeolite. This is ascribed to the proton attack
of the zeolite surface by the chemisorbed HCF− ion pair. Under these preparation conditions, the zeolite structure is fully
preserved. Such enhanced acid properties are traduced by a significant increase in the yield of methyl tert-butyl ether (gas
phase reaction). ©1999 Elsevier Science B.V. All rights reserved.
Keywords: ZSM-5 zeolite; Mild doping with F and subsequent stepwise activation at high temperature; Enhanced acidic properties; Enhanced
activity in the MTBE synthesis
1. Introduction
2. Experimental
2.1. Catalyst preparation
(i) The acid form of the H-ZSM5 was prepared by
repeated ion exchange of the commercially available
Na-ZSM5 zeolite (Zeocat PZ 2/30, Na form, powder,
Chemie Uetikon, Switzerland) with a 10 wt.% solution
of ammonium chloride at 80C with stirring. Each
treatment lasted for 1 h, after which the used solution
was decanted and fresh solution added (1 g of zeolite
in 10 ml solution). The procedure was repeated 4–5
times, after which the solid was washed on the filter
several times with water and dried at 120C. The
acid form was generated by activation at 450C in air
overnight. The final catalyst (extrudates), hereafter referred
to as H-ZSM5, was obtained
4楼2008-05-26 09:13:59
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖

ydx19

铁杆木虫 (知名作家)

氨交换,然后高温焙烧后就得到H型的ZSM-5了
5楼2008-05-31 14:33:21
已阅   回复此楼   关注TA 给TA发消息 送TA红花 TA的回帖