¡¾ÇóÖú¡¿CMS Graphite °ëµç³Ø²âÊÔÇóÖú ÒÑÓÐ3È˲ÎÓë
|
||||
|
Çë´ó¼Ò¸øÒ»Ð©Ö¸µ¼ºÍ°ïÖú£¬Ð»Ð»¡£ ÎÒ×î½üÔÚ×öһЩ¹è²ÄÁÏµÄµç³Ø¹¤×÷£¬ÀûÓÃŦ¿Ûµç³ØÀ´½øÐÐÑо¿£¬ÔÚ×ö×Ô¼ºµÄ²ÄÁÏǰ£¬ÏÈÂòÁËÏÂMTI¹«Ë¾µÄLi-Ion Battery Anode -Copper foil double side coated by CMS Graphite £¨¾ÍÊÇʯīÕý¼«²ÄÁÏ£©×öһЩ±ê×¼»¯¡£ÕâÖмäÓöµ½ºÜ¶àÎÊÌ⣬ºÜ·Ñ½â£¬ËùÒÔÏò´ó¼ÒÇóÖú¡£ ÉÌÒµ»¯µÄCopper foil double side coated by CMS GraphiteµÄÖ¸±êÈçÏ£º • Current collector (substrate): Copper foil, 9 micron • Anode material: CMS Graphite • Double Side Density: 140-160 g/m2 • Length: 222mm • Width: 168mm • Thickness: 0.2mm ( double side coated ) • Net Weight: 0.52 oz/sheet • Double side coated ÎҵIJÙ×÷¹ý³ÌÈçÏ£º £¨1£© µç³Øµ×¸Ç£¨SS316 bottom part£¬ connected to cathode£© £¨2£© ·ÅÈëʯīµç¼«£¨ÆäÖÐÒ»ÃæÊ¹Óõ¶Æ¬Ð¡ÐĹÎÈ¥£©£¬µÎ¼ÓÔ¼50 ΢Éýµç½âÒº£¨ LiPF6£¬ EC+DMC+DEC=1:1:1£©£¨ÒÉÎÊ£¬µç¼«ºÍµç³Ø¸ÇµÄ·ÅÖÃÊÇ·ñ»áÓ°ÏìÐÔÄÜ£© £¨3£© ·ÅÈë¸ôĤ£¬µÎ¼ÓÔ¼50 ΢Éýµç½âÒº£¨ LiPF6£¬ EC+DMC+DEC=1:1:1£©£¬ÈóʪÇé¿öÁ¼ºÃ £¨4£© ¼ÓÈëï®Æ¬×÷Ϊ¶Ôµç¼«£¨ÀïÃæÉÏÓÐÉÙÐíºÚµã£©£¬µÎ¼ÓÔ¼50 ΢Éýµç½âÒº£¨ LiPF6£¬ EC+DMC+DEC=1:1:1£©£¬ÈóʪÇé¿öÁ¼ºÃ £¨5£© ¼ÓÈëµæÆ¬ºÍµ¯Æ¬£¬¸ÇÉÏµç³Ø¸Ç£¨SS316 bottom part£¬connected to anode£© £¨6£© ë²Æø·ÕϾ²ÖÃ30min, £¨7£© ѹƬ£¬100MPa, 30s ¾²ÖÃ10-24Сʱºó£¬Ê¹ÓÃÔ¼1CµÄµçÁ÷£¬ÏȺãµçÁ÷³äÖÁ3.0 V, ÔÙºãµçÁ÷·ÅµçÖÁ0.005 V£¬ ¹Û²ìµÄÏÖÏó£ºµç³ØÈÝÁ¿ºÜµÍ£¬³ä·Åʱ¼ä¶¼ºÜ¶Ì£¨1CϽöΪÊýÊ®Ã룩 ÒÔÉϾÍÊÇÎÒµÄʵÑé²Ù×÷ºÍ½á¹û£¬Çë´ó¼Ò¸øÓè°ïÖú£¬±¾ÈËÐÂÊÖ£¬¸Ðл´ó¼ÒµÄÖ¸µ¼£¬Ï£Íû¿ÉÒÔÔçЩÈëÃÅ¡£Ð»Ð»´ó¼Ò£¡ |
» ÊÕ¼±¾ÌûµÄÌÔÌûר¼ÍƼö
ï®Àë×ÓŦ¿Ûµç³Ø |
» ²ÂÄãϲ»¶
ÄÏ´ó»¯Ñ§µ÷¼Á
ÒѾÓÐ11È˻ظ´
ÁòËáÄÆÈÜҺŨ¶ÈÓëÃܶÈÇúÏß
ÒѾÓÐ0È˻ظ´
·ÖÎö»¯Ñ§ÂÛÎÄÈóÉ«/·ÒëÔõôÊÕ·Ñ?
ÒѾÓÐ111È˻ظ´
0703µ÷¼Á
ÒѾÓÐ4È˻ظ´
1
ÒѾÓÐ21È˻ظ´
0703 µ÷¼Á
ÒѾÓÐ5È˻ظ´
ÕÐÊÕ
ÒѾÓÐ0È˻ظ´
Î÷ÄÏij211ÕÐ27½ì²©Ê¿
ÒѾÓÐ30È˻ظ´
´óÁ¬¹¤Òµ½ÜÇà/³¤½ÍŶÓ-ÉúÎïÖʲÄÁÏ-´¢ÄÜµç³Ø·½ÏòÕÐÊÕ2026¼¶²©Ê¿Éú
ÒѾÓÐ0È˻ظ´
Çóµ÷¼ÁÒ»Ö¾Ô¸º£´ó£¬0703»¯Ñ§Ñ§Ë¶304·Ö£¬Óдó´´ÏîÄ¿£¬Ëļ¶Òѹý
ÒѾÓÐ6È˻ظ´
» ±¾Ö÷ÌâÏà¹ØÉ̼ÒÍÆ¼ö: (ÎÒÒ²ÒªÔÚÕâÀïÍÆ¹ã)
» ±¾Ö÷ÌâÏà¹Ø¼ÛÖµÌùÍÆ¼ö£¬¶ÔÄúͬÑùÓаïÖú:
¹ØÓÚ°ëµç³ØµÄÒÉ»ó
ÒѾÓÐ11È˻ظ´
Ŧ¿Û°ëµç³Ø ʯī
ÒѾÓÐ21È˻ظ´
ÇóÖú¸ôĤºÚµãµÄ²âÊÔ
ÒѾÓÐ4È˻ظ´
CuZnSnSSe ½øÐÐSe´¦ÀíÓõ½µÄgraphite box ÊÇʲô£¿
ÒѾÓÐ5È˻ظ´
¡¾ÇóÖú¡¿Çë½Ì¸ôĤÉϵĺڵãÎÊÌâ
ÒѾÓÐ7È˻ظ´

lyang27
½ð³æ (ÕýʽдÊÖ)
- Ó¦Öú: 5 (Ó×¶ùÔ°)
- ½ð±Ò: 6343.1
- É¢½ð: 63
- ºì»¨: 2
- Ìû×Ó: 439
- ÔÚÏß: 587.4Сʱ
- ³æºÅ: 568058
- ×¢²á: 2008-06-03
- רҵ: µç»¯Ñ§
¡ï
Сľ³æ(½ð±Ò+0.5):¸ø¸öºì°ü£¬Ð»Ð»»ØÌû
Сľ³æ(½ð±Ò+0.5):¸ø¸öºì°ü£¬Ð»Ð»»ØÌû
|
Some suggestions: 1. Use only one side coated CMS, facing Lithium. 2. Discharge (intercalate Li into graphite) the CMS-Li to 0.001V with 1/20 C current 3. Charge (De-intercalate Li) to 1.3 V with 1/20 C current 4. Repeat the cycle twice 5. Cycle the half cell with current density whatever you want. |
4Â¥2011-12-28 06:37:31
wangwenj123
ľ³æ (ÖøÃûдÊÖ)
- Ó¦Öú: 8 (Ó×¶ùÔ°)
- ½ð±Ò: 12599
- ºì»¨: 5
- Ìû×Ó: 2157
- ÔÚÏß: 1000.9Сʱ
- ³æºÅ: 949905
- ×¢²á: 2010-01-28
- ÐÔ±ð: GG
- רҵ: µç·Óëϵͳ
¡ï
Сľ³æ(½ð±Ò+0.5):¸ø¸öºì°ü£¬Ð»Ð»»ØÌû½»Á÷
Сľ³æ(½ð±Ò+0.5):¸ø¸öºì°ü£¬Ð»Ð»»ØÌû½»Á÷
|
Ä㾹ȻÓÃ1CµçÁ÷£¬²¢ÇÒ»¹³äµ½3.0V¡£¡£¡£¡£¡£¡£¡£¡£¡£¡£¡£¡££¡ |